Spinning of Petroleum based Isotropic Pitch by Melt-blown Method

  • Received : 2001.08.13
  • Accepted : 2001.12.20
  • Published : 2002.03.30

Abstract

Petroleum based isotropic pitch was spun into short fiber by melt-blown spinning technology. The processing parameters chosen were air velocity, die temperature, and throughput rate of the pitch within the ranges of experimental tolerances. The fiber diameter was reduced to $6{\mu}m$ by increases of hot air velocity, and spin die temperature. Also, the fiber diameter was strongly dependent on the throughput rate of the pitch and jet speed of hot air through the spinnerets. Even fibers with $10{\mu}m$ diameter were produced at throughput rate of $0.17g/min{\cdot}hole$ and at die temperature of $290^{\circ}C$.